Introduction

Heusler compounds are an interesting class of materials with a wide variety of useful properties for technological applications1,2,3. Cobalt-based Heusler alloys, Co2XY (X = transition or rare earth elements and Y = Si, Al, Ge and Sn) have been the subject of extensive studies in the context of spintronics over the last decade4,5,6. Some of these alloys exhibit half-metallic behavior with 100% spin polarization at the Fermi edge, and have applications in spintronics7,8,9. The Co2TiGe (CTG) compound is one of most promising candidates for spin manipulation because it is a half-metallic compound with a Curie temperature higher than 300 K10,11,12. A number of structural, magnetic, and electrical transport studies have been carried out in bulk CTG10,11,12,13. Recently, band structure calculations revealed that CTG is a Weyl semimetal (WSM) with broken time reversal symmetry due to ferromagnetism14,15. Interestingly, the momentum space locations of the Weyl nodes in CTG can be controlled as a function of the magnetization direction. WSM can be realized in materials either by breaking crystal inversion symmetry, time reversal symmetry, or both16. In inversion symmetry breaking materials, angle resolved photo emission spectroscopy, and transport measurements have provided evidence for Weyl fermions and surface Fermi arcs that are characteristics of WSMs17,18,19,20. In CTG, which is a magnetic WSM, the ferromagnetic behavior produces negative magnetoresistance (MR) and anomalous Hall effect, which have been reported in the bulk15,21,22,23. So, understanding the WSM behavior in half-metals solely based on transport properties will be challenging. In addition, the calculated momentum locations of the Weyl nodes in CTG with (001) magnetization are considerably far away (>250 meV) from the Fermi energy, so significant effects of Weyl behavior in transport will be difficult to observe15,21. In this article, we have grown CTG films using molecular beam epitaxy (MBE). We have observed semimetallic behavior, low charge carrier density, negative MR with sharp cusps at low magnetic fields, and small anomalous Hall conductivity, which depends on the longitudinal conductivity in the temperature range 5 to 300 K. These observed properties in nanostructured thin film are completely different from the reported bulk properties.

As shown in Fig. 1(a), CTG consists of four sets of interpenetrating face-centered cubic sublattices with the space group Fm\(\bar{3}\)m. Smooth and continuous thin films are obtained using MBE deposition, as described in the experimental section. The typical thickness of the deposited films is 50 nm (Supplementary Information S1). The X-ray diffraction pattern recorded for CTG film is shown in Fig. S2, which can be indexed based on cubic L21 structure. The detailed overview of the structural characterization of CTG is described in supplementary information. The value of the lattice constant is 5.81 Å, which matches well with previously reported values in literature10,11,12. The chemical ratio of Co:Ti:Ge is equal to 50:24.8:25.2, which is very close to the stoichiometric ratio (Fig. S3). From the magnetic measurements, saturation magnetic moment per formula unit (f.u.) calculated is 1.9 µB at 10 K, comparable to the theoretical value of 2 µB/f.u2. At 300 K, the magnetic moment drops to 1.5 µB/f.u. (Fig. S4). The magnetization versus temperature with an applied field of 500 Oe is shown in Fig. S5. A Curie temperature of 379 K is observed, while the reported values vary from 380 to 391 K10,11,12.

Figure 1
figure 1

Lattice Structure and Electrical Transport. (a) The Fm \(\bar{3}\)m lattice structure of Co2TiGe (b) Resistivity variation of CTG thin film with temperature. Inset shows the resistivity variation and the fit for T > 200 K. The resistivity fitting of CTG film for temperature (c) less than 80 K and (d) 80 to 200 K.

Figure 1(b) displays the temperature dependence of the zero-field longitudinal resistivity, ρxx(T) from 10 to 300 K. Maximum resistivity is observed around 200 K. The temperature dependence of resistivity below 200 K shows a metal-like conduction22. For temperatures above 200 K, the resistivity is decreased. Such change of resistivity can only be found in semimetals or narrow gap semiconductors23,24,25,26. The logarithm of resistivity behavior above 200 K plotted against 1/T as shown in the inset can be fitted with a straight line, yielding an effective energy gap of 24 meV27,28. For temperatures lower than 200 K, the temperature dependence of resistivity can be written as \({\rho }_{XX}=\,{\rho }_{XX0}+{\rho }_{e-e}+{\rho }_{e-ph}+{\rho }_{e-m}\). Here, the term ρXX0 is the residual resistivity which arises due to the impurity scattering; ρe−e is the resistivity contribution from electron-electron scattering, which has a T2 dependence at low temperature; ρe−ph term is due to electron-phonon scattering which has a T dependence at higher temperature and a T5 dependence at low temperature; the term ρe−m is contributed by electron-magnon (e-m) scattering. For a normal ferromagnetic material, electron-magnon scattering leads to T2 dependence of the resistivity29. However, in half-metallic ferromagnets, a band gap for minority charge carriers at Fermi level prohibits one magnon scattering. In such a case, ρe−m has a T9/2 dependence at low temperature and a T7/2 dependence at high temperature29,30. The T3 resistivity dependence has been predicted in some half-metallic systems, and such scattering process is called anomalous single magnon scattering29. In Co-based Heusler alloys, a T3 dependence has not been observed13,29. In our thin films, we have divided resistivity below 200 K into two regions, T < 80 K and T > 80 K. T < 80 K region is fitted with the relation ρXX = ρXX0 + AT2 + BT4.5 + CT5 as displayed in Fig. 1(c). From the best fit, we have obtained ρXX0 = 260 μΩ cm, A = 8.31 × 10−10 μΩ cm K−2, B = −3.24 × 10−14 μΩ cm K−4.5 and C = 2.89 × 10−15 μΩ cm K−5. The very small value of coefficient C indicates considerable phonon drag effects in our system. The small value of coefficient A indicates weak electron-electron scattering and the small negative value of coefficient B hints weak negative contribution from double magnon scattering. Figure 1(d) shows the resistivity fitting for the resistivity above 80 K and less than 200 K. We have fitted this region with the relation, ρXX = ρXX0 + DT + ET3.5 with the values ρXX0 = 260 μΩ cm, D = 5.85 × 10−8 μΩ cm K−1 and E = −5.11 × 10−14 μΩ cm K−3.5 respectively. The small value of E indicates weak negative double magnon scattering contribution in our alloy at higher temperature. Thus, the transport is mainly dominated by electron-phonon scattering and weak electron-electron and electron-magnon scatterings. The resistivity behavior observed in our CTG thin films is different than that previously reported for cobalt-based Heusler alloys. First, we have observed a semimetallic behavior with a very small energy gap below the Curie temperature. Second, we have not observed any upturn in resistivity at low temperature. Previous studies have shown a resistivity upturn in the temperature range of 5 to 50 K. It has been suggested that such a minimum should occur due to a localization effect at low temperature29,31.

Figure 2(a) summarizes the temperature dependence of longitudinal magnetoresistance calculated using the formula \(\frac{[\rho (B)-\rho (0)]}{\rho (0)}\times 100 \% \), where ρ(B) and ρ(0) are the resistivities at magnetic field B and zero field, respectively, and the field was applied parallel to the current as shown in the inset. The magnitude of MR is less than 0.5% at a 4 T magnetic field. The MR curves display positive cusp from 5 to 300 K at low field (<0.5 T). For fields greater than 0.5 T, MR is temperature dependent and slowly varying with magnetic field. A negative MR has been measured for temperatures up to 300 K. However, at 300 K, MR tends to go positive after a field of 0.5 T. The maximum negative MR is observed around 100 K and beyond that negative MR decreases in magnitude, as shown in Fig. 2(b). Previous studies on Co2TiGe have not demonstrated such sharp peak-like behavior at a low magnetic field. Indeed, they have shown non-saturating negative MR with temperature9,22,32 due to reduction of spin flip scattering and also, reduction of electron-magnon scattering. Studies have also shown the linear magnetic field dependence of MR33,34. Though negative MR has been reported in bulk CTG, it is interesting that our CTG films exhibit sharp peaks in MR behavior even up to 300 K in contrast to the bulk behavior12. The saturation magnitude of the MR shows an increase from 5 to 100 K that then decreases as the temperature increases above 100 K.

Figure 2
figure 2

Magnetoresistance. (a) Magnetoresistance of CTG thin film when the magnetic field is applied along the direction of the current at different temperatures (Inset shows the measurement scheme). (b) MR variation of the thin film with temperatures for the four fields.

The magnetoconductance (MC) of CTG thin films is calculated as conductance at the applied field minus conductance at zero field. The increase in MC at the lower magnetic field is displayed in Fig. 3(a) at different temperatures from 5–300 K. At all temperatures, the MC curves are dominated by weak localization effects leading to a sharp downward cusp which indicates a large increase in conductance at low magnetic fields. The saturation magnitude of the conductance increases until the temperature is 100 K and then shows a reduction. Dugaev et al.35 have theoretically demonstrated that in the case of ferromagnets, spin–orbit interaction can only give negative magnetoresistance, which means MC increases with increasing magnetic field. The quantum corrections to the MC in ferromagnets when the external magnetic field applied parallel to the current can be described by the Al’tshuler and Arnov (AA) equation36. The conductance has a logarithmic dependence on magnetic field \(\,{\rm{\Delta }}G=\frac{{e}^{2}}{2{\pi }^{2}\hslash }\,\mathrm{ln}(1+\frac{\beta e{t}^{2}{B}^{2}}{4\hslash {B}_{\varnothing }})\), where t is film thickness \(\hslash =h/2\pi \), h is Planck’s constant, e is the electronic charge, β is related to the ratio of mean free path and film thickness, and B is the effective dephasing field from which effective dephasing length (L) can be estimated as \({B}_{\varnothing }=(\hslash /4e{L}_{\varnothing }^{2})\)37. The MC behavior at all temperatures fit well to the Al’tshuler and Arnov equation (shown in red solid line) at lower field as illustrated in Fig. 3(a). From the fits, we have calculated the dephasing length at different temperatures, which are plotted in Fig. 3(b) together with the fitting parameter β. β varies from ~0.1–0.4; these values are close to the upper bound of β in the Al’tshuler-Arnov regime, 1/3. The dephasing length shows an anomalous behavior as a function of temperature. At 5 K, the dephasing length is 270 nm. It increases with temperature, reaches a maximum value of 450 nm at 100 K, and then decreases with a further increase in temperature. This temperature dependence of dephasing length suggests the influence of other scattering mechanisms which affect the phase coherence apart from Nyquist mechanism38.

Figure 3
figure 3

Parallel Transport. (a) Variation of magnetoconductance of CTG thin films at different temperatures for low fields (AA equation fitting are shown in solid red line). (b) Variation of dephasing length and the fitting parameter β with the temperature.

To get further insight, we have carried out Hall resistivity measurements. Figure 4(a) presents Hall resistivity (ρXY) at different temperatures in the field range of ±4 T. At a particular temperature, as the applied magnetic field is increased from zero, ρXY initially increases with magnetic field before settling at saturation (Fig. S6). The total resistivity for a magnetic system can be expressed as, \({\rho }_{XY}={R}_{0}B+{\mu }_{o}{R}_{s}M\) where R0 and RS are ordinary and anomalous Hall coefficients, M is the magnetization, and μo is the relative permeability29,39. The first term is the ordinary Hall resistivity that arises due to Lorentz force, and the second term is anomalous Hall resistivity (ρAHE) which originates from the intrinsic magnetization. From the theoretical perspective, ρAHEconsists of both an intrinsic band structure dependent contribution and an extrinsic skew and side jump scattering contribution. The anomalous Hall resistivity can be extracted by a zero-field extrapolation of high field ρXY data. At a given temperature, the slope of the high field linear part of the ρXY plot is equal to R0. We have obtained positive values of R0 which increase with temperature. Based on the one band model, we have calculated the effective charge carrier density using the formula n = 1/(R0 e)29,40. The corresponding effective carrier concentration is 6.86 × 1021 per cm3 at 5 K. The mobility is another important quantity for the charge transport which can be expressed as \(\mu =\frac{{R}_{o}}{{\rho }_{xx}}\). The value of mobility is 35 cm2V−1s−1 at 5 K. The temperature dependence of anomalous Hall resistivity and saturation magnetization is displayed in Fig. 4(b). The value of ρAHE increases as we decrease the temperature from 300 to 5 K, similar to the temperature dependence of magnetization, which clearly shows the dependence of anomalous Hall resistivity on the magnetization. To gain more understanding about the dependence of anomalous Hall resistivity on different scattering mechanisms, we have investigated how ρAHE scales with longitudinal resistivity. The scaling relation of ρAHE with ρxx for Heusler alloys has been analyzed by Vidal et al.39. The scaling relation can be written as, \({\rho }^{AHE}=(a{\rho }_{XX0}+b{\rho }_{XX0}^{2})+(a+2b{\rho }_{XX0}){\rho }_{XX(T)}+b{\rho }_{XX(T)}^{2}\), where ρXX0 is the residual longitudinal resistivity and ρXX(T) is temperature dependent resistivity, a is the parameter which contains information about skew-scattering and b is related to intrinsic mechanism which contains also side jump contribution. The fitting is displayed in Fig. 4(c). From the fitting, we have obtained the value of a = 0.12 and b = −5 × 10−4 (μΩ cm)−1 respectively. Such negative values of b have been reported by Vidal et al.39 and Imort et al.41 in cobalt-based Heusler alloys because of negative scattering potential. In our thin film, though the value of b is smaller than the value of a, the fit illustrated that it could not be negligible. That means b which has information about side jump scattering and intrinsic mechanism contribute to anomalous Hall resistivity along with skew scattering. Hence, anomalous Hall resistivity in our thin film is contributed by extrinsic and intrinsic scattering mechanisms. The Hall conductivity is calculated using the formula, \({\sigma }_{XY}=-\,\frac{{\rho }_{XY}}{{\rho }_{XX}^{2}}\), where ρXX is longitudinal resistivity42 as displayed in Fig. 1(b). The field dependence of Hall conductivity is shown in Fig. 5(a). The anomalous Hall conductivity (AHC) can be extracted from this plot by extrapolating the high field Hall conductivity to zero field. We have obtained a value of 27 S/cm at 5 K. The dependence of AHC (σAHC) on longitudinal conductivity (σxx) is illustrated in Fig. 5(b) which demonstrates a nonlinear dependence of σAHC on σxx. Further, the anomalous Hall conductivity decreases while increasing the temperature similar to the behavior of magnetization with the temperature (Fig. 4(b)), which clearly demonstrates the dependence of magnetization on σAHC in our thin film. However, previous studies have shown that intrinsic anomalous Hall effect has either a linear or a non-linear dependence on magnetization43,44. The longitudinal conductivity in our film is in the range observed in the dirty regime of other ferromagnets45,46, but the scaling relation, σAHC  σXX does not fit to our data. From Fig. 4(c), it is evident that the anomalous Hall resistivity scales with longitudinal resistivity. Such scaling of ρAHE is neither linear nor quadratic on ρXX but combination of both linear and quadratic in ρXX. Further, AHC strongly depend on σXX as the temperature increases. Hence, anomalous Hall resistivity and the small value of AHC observed in our thin film is contributed by the skew-scattering, side-jump scattering, and intrinsic mechanism47,48.

Figure 4
figure 4

Hall Resistivity. (a) Hall resistivity as a function of the magnetic field of CTG thin film (Inset shows the Hall measurement scheme, where current is applied on x-direction and measured Hall voltage is perpendicular to both applied magnetic field and current). (b) Variation of anomalous Hall resistivity and saturation magnetization with temperature. (c) Plot of anomalous Hall resistivity as a function of longitudinal resistivity. The line is a fit to the data points using the equation, \({\rho }^{AHE}=(a{\rho }_{XX0}+b{\rho }_{XX0}^{2})+(a+2b{\rho }_{XX0}){\rho }_{XX(T)}+b{\rho }_{XX(T)}^{2}\).

Figure 5
figure 5

Hall Conductivity. (a) Variation of Hall conductivity with temperature and field. (b) Anomalous Hall conductivity as a function of longitudinal conductivity.

In summary, we have systematically investigated the structural, magnetic, electrical and magnetotransport properties of Co2TiGe thin films. We have demonstrated the ferromagnetic and semimetallic nature of CoTiGe thin films. The detailed analyses of parallel magnetoresistance at lower fields establishes the localization correction. The shorter dephasing length has been obtained at lower temperature. The dependence of anomalous Hall conductivity on longitudinal conductivity indicates the contributions to the AHC may arise due to both intrinsic and extrinsic mechanisms.

Sample Preparation

Co2TiGe (CTG) thin films were grown using molecular beam epitaxy deposition. The base pressure inside the chamber was below 9 × 10−10 Torr and less than 5 × 10−9 Torr during the film deposition49,50. Polished silicon (100) substrates were used for the film deposition. Prior to deposition, the silicon substrate was cleaned with distilled water, isopropyl alcohol, and acetone. After cleaning, the substrate was etched in 2% hydrofluoric acid to remove oxide from the surface. Wafers were placed inside high vacuum and preheated at 473 K for 20 minutes. A 5 nm buffer layer of magnesium oxide was deposited. A stoichiometric ratio of Co, Ti, and Ge was simultaneously deposited; with film composition and uniformity controlled by a quartz crystal rate monitor and a low deposition rate of 0.3–0.5 Å/s. The temperature of the growth was maintained at 573 K. Films were grown with a thickness of 50 nm. After growth, the films were annealed in situ at 773 K for 2 h. Finally, 5 nm MgO was deposited as a cap layer.

Thin Film Characterization

The morphology of the thin films was examined by scanning electron microscopy (SEM) (JEOL JSM-5910LV). The composition was determined by energy-dispersive X-ray (EDX), [JEOL JSM-5910LV] spectroscopy. The crystal structure was determined by x-ray diffraction analysis (XRD) using a Thermo/ARL X’TRA, (Cu-Kα) diffractometer. The magnetic measurements were carried out using a Quantum Design vibrating sample magnetometer (VSM).

Transport Measurements

To measure transport properties of thin films, Hall bar devices were grown using metal contact masks with dimensions 500 × 500 μm and 50 nm thick. Gold-wire electrical leads were attached to the samples using indium. The longitudinal resistivity and Hall resistivity of the samples were measured using a physical properties measurement system (PPMS) AC Transport with horizontal rotator option.